Alumina toughness Zirconia (ZTA) |
|
Characteristics |
Item |
Value |
Unit |
|
Mechanical Characteristics |
Colour |
White |
|
Density |
4.2 |
g/cm3 |
|
Bending Strength |
550 |
MPa |
|
Compressive Strength |
2,900 |
MPa |
|
Elastic Modulus |
360 |
GPa |
|
Fracture Toughness |
5~6 |
MPam1/2 |
|
Weber Coefficient |
15 |
M |
|
Vickers Hardness |
1,600 |
HV0.5 |
|
Thermal Characteristics |
Coefficient of Line Thermal Expansion |
8.3 |
10-6K-1 |
|
Thermal Conductivity |
27 |
W/mK |
|
Thermal Shock Resistance (Put in Water) |
300 |
?T°C |
|
Max Working Temperature |
1,500 |
°C |
|
Electrical Characteristics |
Volume Resistance at 20°C |
>1014 |
?cm |
|
Dielectric Strength |
9×106 |
V/m |
|
Dielectric Constant |
10.6 |
εr |
|
One MHZ Dielectric Loss Angle at 20°C |
0.0005 |
tanδ |
|
Chemical Characteristics |
Nitric Acid (60%) 90°C |
- |
WTLossmg/cm2/day |
|
Sulphuric Acid (95%) 95°C |
- |
|
Caustic Soda (30%) 80°C |
- |
The chart is intended to illustrate typical properties of ZTA ceramic. Engineering data is representative. Property values vary somewhat with method of manufacture, size, and shape of part. |